Giải pháp
Horse Construction cung cấp đầy đủ các loại vật liệu gia cố kết cấu với hỗ trợ kỹ thuật, hỗ trợ tài liệu, hỗ trợ sản phẩm, hỗ trợ phần mềm, hỗ trợ dự án.
For cracks in concrete beams with width of 0.2-mm, besides epoxy resin pressure grouting according to the two methods, CFRP is bonded to seal the surface. Reinforced concrete beams are reinforced by CFRP sheets at the bottom of the mid span.

Treatment measures for cracks in plastering layer
Use the cutting machine to cut out the plaster empty drum part, then clean the loose plaster clean and scour out the floating ash with clean water, sweep 108 glue mud on the wall surface and the plastering layer, and smooth out the light by the same marking mortar. Spray water for 7 days. After drying, put 100 wide crack resistant mesh on the old and old plastering, then scrape the elastic putty.
Treatment measures for wall cracks
The method of high strength cement slurry is used in the crack larger than 1.5mm; for the 100 wide plastering layer on both sides of the crack under the crack less than 1.5mm, the base treatment is carried out, and the 100 wide crack proof mesh cloth is attached, and the light is smooth and the elastic putty is used with the same marking mortar.
Treatment measures of floor cracks
The cracks on precast concrete floors are reinforced with carbon fiber sheets at the bottom of precast concrete floors.
The cracks on the surface of the cast-in-place plate are not less than 20mm and 15 mm grooves on the surface of the floor, and the groove width is not less than that of 15 mm. Then the modified epoxy resin material is filled and the carbon fiber composite material is attached to the surface.
Treatment measures for cracks on the beam
1. The crack width is less than 0.2mm, which is a harmless crack. Because of the remarkable self healing capacity of the compensated shrinkage concrete, the two surfaces of the fractured surface can be cemented into one by the expansive hydrate blockage, even in some seepage cracks. Therefore, when the crack width is less than 0.2mm, surface treatment can be carried out. A steel wire brush is used to remove the concrete surface attachments. After rinsing with water, the surface treatment material (elastic coating waterproof material, polymer mortar and so on) is disposed in accordance with the material use description, and the cracks and the surrounding parts are evenly coated.
2. For the deep cracks which are difficult to surface treatment, first chisel the crack into a "concave" groove, clean it with water, then use the cement paste with 10% expansive agent, brush the surface of 1 ~ 2mm on the surface, and then apply 4 ~ 5mm cement mortar after the paste layer is slightly dry. Mix ratio: cement: expansive agent: Sand: water = 1:0.10:2.0: (0.35 ~ 0.38). Finally, 12 hours after compaction, light harvesting and plastering for watering maintenance.
3.The penetrative cracks can be repaired by epoxy resin pressure grouting. At the distance of 2 to 5cm on both sides of the crack, the distance between the cracks is set up and the distance of the injection port is set up. The seaming slurry is made up. After leveling, the cracks are smear along the surface of the crack, the cracks are closed, the injection mouth is left out. The grouting material is inserted into the injection nozzle to press the grouting material into the crack. After 1 days of general injection, the glue will be removed and the surface will be cleaned up after the glue is solidified.
4.For cracks in concrete beams with width of 0.2-mm, besides epoxy resin pressure grouting according to the two methods, CFRP is bonded to seal the surface. Reinforced concrete beams are reinforced by CFRP sheets at the bottom of the mid span.
Bạn có thể tìm thấy mọi thứ bạn cần ở đây. Hãy tin tưởng và thử nghiệm các sản phẩm này, bạn sẽ thấy sự khác biệt lớn sau đó.
Lớp bọc sợi carbon đơn hướng, cường độ cao được bão hòa trước để tạo thành lớp bọc polyme gia cường sợi carbon (CFRP) dùng để gia cố các cấu kiện bê tông kết cấu.
Tấm polyme gia cường sợi carbon (CFRP) ứng suất trước dùng để gia cố sàn, dầm nhằm tăng độ cứng, giảm biến dạng và độ võng của các cấu kiện, giảm vết nứt, tránh và ngăn ngừa nứt.
Keo phun vết nứt bê tông Horse HM-120L là loại keo epoxy dùng để sửa chữa vết nứt bê tông bằng cách tiêm. Keo epoxy có tính thẩm thấu cao. Tiêm vết nứt ở áp suất thấp trong bê tông kết cấu.